I couldn’t help but trying Calvin’s super-coated carbon tissue again. This is the DAS-sensitized tissue with another unpigmented gelatin layer on top of it, that’s supposed to all but solve the problem of the tonal threshold. Contrary to my earlier attempts, this time it seems to be working…?
My previous attempts are described in two consecutive blog entries (here and here). They boil down to a grand…failure. I had problems with the tissue not making a good transfer, and insofar as it worked, the tonal threshold behavior wasn’t any better than with an identical tissue without the top layer. Bummer.
I kind of abandoned it in wait for my luck to turn. Or my stubbornness to get the better of me, I’m not sure. Either way, recently there was this post by Vlad Yurkov that showed a rather spectacular application of Calvin’s ‘super emulsions’. Honestly, credit where it’s due – those examples blew me off my socks. Not just the end result, but also the diligence and commitment of Vlad that went into mastering the process. Awesome!
And…inspiring. So I just had to try it. But I didn’t (and still don’t, quite) have the time to do rigorous testing. Instead, I just cooked up something quickly and haphazardly – just…I don’t know. Kind of randomly hoping it would work.
I made a simple glop using 8% w/v gelatin, 12% w/w (per gelatin) Talens India ink and 4% w/w DAS. I also made a clear supercoat layer following a tidbit dropped by Vlad: 1% w/v gelatin in water. That’s it. I poured the pigmented layer to a height of ca. 0.8mm (this is on the thin side; I mostly aim at 1.0-1.1mm), then let it set and poured the clear supercoat layer on top of it.
Here I have to distinguish between two rounds of experimentation. The first round used the 1% gelatin in water supercoat as indicated above. I coated this on top of the pigmented tissue to a height of approx. 0.4mm. To spread it, I used a glass stirring rod as a puddle pusher, simply holding it on both ends and carefully moving it across the surface of the tissue. Frankly, this approach doesn’t work very well. The watery-thin supercoat emulsion tends to easily run off the edges of the pigmented tissue, creating a mess and also causing variation in how much of it actually ends up on the tissue (thus affecting printing characteristics).
In a second experiment, I used Calvin’s approach of diluting the supercoat emulsion with ethanol. In this case, I made a supercoat with a much higher gelatin content: 4% w/v in water, to be diluted 1:1 with ethanol, ending up with 2% w/v gelatin in the supercoat as actually coated. Because this is much more runny and has lower surface tension, I could not possibly coat it to the same 0.4mm height and instead ended up at somewhere around 0.2mm or so. Hence, the final amount of supercoat gelatin was approximately the same as in the initial experiment.
Well, honestly, there was another difference between both experiments: I used Talens India ink in the first one, but used Kremer XSL Black ‘just add water’ pigment for the second. This may be relevant as we will see later on, although I’m not entirely sure.
Okay, full disclosure, the second experiment differed in several ways from the first. Due to the use of ethanol to dilute the supercoat emulsion, coating became ‘a bit’ tricky. The puddle-pusher approach really didn’t cut it and in some brief mucking about, I found that simply spreading the emulsion with my fingers was the most convenient approach. I’ve since done the same with a third batch (no prints yet; they’re drying) and no ethanol in the supercoat, and this confirms that simply spreading the supercoat emulsion by hand (literally) so far works best for me.
Also, the final transfer to paper was on a different medium for experiment #2 than for one, because I felt like giving transfer to baryta photo paper a try (which worked great, but I dislike the result).
To summarize, some parameters for both experiments:
| Experiment #1 | Experiment #2 | |
|---|---|---|
| Pigment | Talens India ink | Kremer XSL Black |
| Pigment load (in relation to dry gelatin weight) | 12% w/v | 1.6% w/v |
| Gelatin in pigmented glop (w/v to water) | 8% w/v | 8% w/v |
| Pour height pigmented layer | ~0.8mm | ~0.8mm |
| Supercoat gelatin concentration | 1% w/v | 2% w/v (after dilution with ethanol before coating) |
| Supercoat height | ~0.4mm | ~0.2mm |
| Supercoat pour technique | Glass stirring rod as puddle pusher | Spread with fingers |
| Final transfer to | Schut Laurier gelatin-sized fine art paper | Fixed-out Ilford Galerie FB baryta silver gelatin paper |
It turns out that the printing characteristics were quite similar, but both tissue types suffered from defects. These defects look perfectly avoidable to me, especially those in experiment #1. But let’s have a look at the final prints, first:


As said, both prints suffer from several problems, most of which are attributable to sloppy technique. This is because I worked quickly, looking for a ‘proof of concept’ and thus cut several corners in various places. These are for the most part, or even entirely, avoidable. Let’s have a look at the problems and known solutions, starting with print #1.
| Problem | Causes / solution |
|---|---|
| Pinholes / white spots | These are in fact bubbles in the tissue. Glop was not allowed to offgas very long, so air remained in it. My normal workflow allows for a longer offgassing time which avoids this problem. |
| Grey ‘halo’ of density around the image | Combination of factors: 1: The negative used here is fairly dense in the highlights, and the supercoat reduces the speed of the tissue. The short-wavelength (365nm) exposure was thus rather excessive and sufficient to actually burn straight through the Rubylith mask around the image. 2: Adding to the above, the supercoat layer did not reach all the way to the edges of the tissue, thinning out towards the edges. This means that some of the exposure especially along the edges penetrated into the pigmented tissue layer, while in the center it mostly kept restricted to the clear supercoat. Solutions involve ensuring the supercoat extends to closer to the tissue edge, print smaller than the side of the tissue to avoid the edges, and simply wipe off non-image gelatin around the image during the warm-water development step. |
| Blisters in high-density areas | While this is not visible in the scan above, it can be seen in the real print. I’ve included an illustration below. I’m frankly not entirely sure where this problem originates from and it only appears on prints from experiment #1. I suspect that nitrogen gas emanating form the pigmented image layer somehow got trapped between the pigmented tissue layer and the clear supercoat layer, causing local and partial delamination of both layers, possibly exacerbated by the strong extent of hardening in high-density areas. The problem did not occur in experiment #2. If/when it pops up again, this may require additional diagnosis and troubleshooting. |
| Yellow staining | I did not clear the DAS stain from either of the prints. Clearing the stain with permanganate removes the stain. Note that the stain can intentionally be left in to add a yellow/orange toning to the image, which can be desirable in some prints. |

Now let’s have a look at the problems with print #2.
| Problem | Causes / solution |
|---|---|
| Overall yellow discoloration of paper base | This is due to the paper base I used how I (mis)handled it. I took some old sheets of very expired Ilford paper out of the back and fixed them out while exposed to regular room light. This has resulted in such a pronounced print-out density that it has contributed significant density (essentially a lumen print). Fixing the paper under safelight conditions avoids this issue. |
| Yellow staining of image area | DAS stain; see comments on same issue in print #1. Avoidable issue. |
| Blistering around hard edges of high density | You have to look really closely to see this; I’ve included an illustration below. The root cause here is inherent to the double-transfer carbon process if the image layer is relatively thick. The high relief makes it difficult to bring all of the image into direct contact with the gelatin layer of the receiver/final transfer paper – especially if that gelatin layer is fairly thin or very hard and thus cannot swell well and conform to the image relief. Solutions are to use a gelatin sizing that’s heavier and unhardened to it swells more and conforms to the image relief, or to use a thinner image layer with less relief. This is possible by increasing pigment load, which would normally create highlight problems, but the clear supercoat layer makes it possible to push the limits on pigment load further. |
| Eddy / flow marks | These are very apparent especially in the upper 1/3 of print #2; see e.g. the patterns in steps 15-19 of the Stouffer. I expect this is due to the use of ethanol to dilute the supercoat emulsion. I added the ethanol at room temperature to the warm gelatin solution, causing instant clouding over of the supercoat emulsion. What apparently happens is a partial and instantaneous hardening of the gelatin. As a result, the solution is no longer nicely homogeneous, but turns into a partial dispersion of gelatin strands. These strands don’t deposit in a neat, even layer like regular melted (dissolved) gelatin. I think that’s what created these patterns: a heavier layer of gelatin strands was deposited locally as I was spreading out the supercoat solution, causing fairly dramatic thickness variations in the dried supercoat layer. In Calvin’s video demonstrating the supercoat procedure, he’s actually pretty careful with how much ethanol he adds – he uses 25-30% (so 3:1 dilution) instead of my 50% (1:1 dilution). I simply pushed beyond the reasonable limits with how much ethanol I added. |

So, lots of problems. You might wonder, anything good to go with that, at all? Well, in fact – yes! Firstly, I noted no transfer issues like I did in the earlier experiments, where the supercoated tissues appeared to exhibit severe issues with adhesion during the warm-water development bath. I still don’t quite know what caused those issues. Calvin hinted that it was the type of gelatin used, but I find that hard to believe, especially since the experiments reported in this blog entry use the exact same gelatin as before – and the same gelatin for both the image layer and the supercoat.
Secondly, highlight rendition of the prints seems very good in the sense that there’s no clearly visible tonal threshold. I’ve had a good look at the matrices before transferring to paper, and with magnification (a loupe) it’s easy to see how in the lightest highlight areas, the unpigmented gelatin forms a first base layer that adds virtually no optical density. This implies that the principle works: the image buildup starts with a colorless gelatin layer that acts as an adhesion layer for the pigmented image layer that comes on top, which effectively shifts the tonal threshold problem into the clear supercoat layer where it remains invisible. The resulting transitions between areas of light tone to ‘paper white’ become smooth. What texture there is to those transitions is limited to the actual image structure – e.g. in this particular scene, the muslin fabric of the shirt.
The tentative success does come at a cost. The tissue becomes horrendously slow. Since the clear supercoat layer needs to be ‘printed through’ before density starts to build, the tissue easily exposes one or two stops slower than comparable tissue without supercoat. This implies that there’s a tradeoff or an optimum that can be found by balancing two effects against each other:
- A thinner supercoat will have less speed loss, but there may be tonal threshold problems
- A thicker supercoat will have considerable speed loss, but avoid a visible tonal threshold
Beyond a certain thickness of the supercoat layer, there’s no added advantage; once the tonal threshold becomes invisible, the target is reached. So the key is to find a thickness (in terms of dry gelatin on the dried tissue) of the supercoat that strikes a balance between these two.
Wondering whether perhaps the apparent success of these recent attempts was due to a thicker supercoat than what I gleaned from Calvin’s manual, I compared them:
| My experiment #1 | Calvin’s manual | |
|---|---|---|
| Gelatin to water | 1% w/v | 0.8% w/v |
| Ethanol dilution | none | 10+3: 1000ml gelatin solution + 300ml ethanol |
| Pour height supercoat | 0.4mm | 0.5mm |
| Gelatin load of dried supercoat | 0.4mg/cm2 | 0.3mg/cm2 |
Turns out that I am indeed using a 33% thicker layer here. However, I doubt this is the only explanation for the better performance, as I have not observed any of the flaking that I got in my earlier attempts. I feel this must be due to a different parameter, but I’ve not figured that out yet. I’m also not sure if I ever will, unless the problem rears its head again. Fingers crossed I’ll never have to find out!
In the meantime, I’ve been printing through the tissues of these two experimental batches. All of these prints demonstrate that the prints shown on this blog entry are representative for how these tissues behave – i.e. the ones shown here are not somehow flukes in either a positive or a negative sense. The inherent problems are there in all prints, but so are the inherent benefits of better highlight rendition.
All in all, very promising in my view, although certainly not ‘ripe’ yet.